12L14 / 11SMnPb30 free-machining steel speeds and feeds

12L14 / 11SMnPb30 (1.0718) free-machining steel is turned at 250-400 m/min (about 820-1,310 SFM) with 0.3 mm/rev using coated carbide, milled in the same range at 0.12 mm/tooth and drilled at 175-300 m/min with 0.2 mm/rev. It is the classic bar stock for screw machines and Swiss-type lathes: sulphur and lead make the chip break on its own into short pieces, so you can run fast and unattended.

Designation
EN 11SMnPb30 / 1.0718 · AISI 12L14
Hardness
160 HB
ISO group
Steel (P)
Turning Vc
250–400 m/min

Which operation are you machining?

Recommended speeds and feeds

Turning

250–400 m/min

0.3 mm/rev

250-400 m/min at 0.3 mm/rev for roughing; for finishing drop the feed to 0.1-0.15 mm/rev and keep the speed high so no built-up edge forms. On screw machines with long bar and small parts, the limit is usually bar rigidity and diameter: on small diameters the spindle runs out of rpm long before the insert reaches its cutting speed.

Milling

250–400 m/min

0.12 mm/tooth

Same 250-400 m/min range at 0.12 mm/tooth. The short chip does not tangle, so generous feeds are fine. For finish facing, a wiper-insert face mill at high speed leaves a very good surface.

Drilling

175–300 m/min

0.2 mm/rev

175-300 m/min and 0.2 mm/rev with a carbide drill. It is one of the easiest steels to drill: chips come out broken even in holes several diameters deep. With an HSS drill, drop to about 40-60 m/min (130-200 SFM).

Threading

88–180 m/min

0.2 mm/rev

88-180 m/min for single-point threading with carbide on the lathe. Cutting or roll-form HSS-E taps work very well thanks to the short chip: around 15-25 m/min with cutting oil.

Starting values for coated carbide in medium cutting. Fine-tune them in the calculator for your tool, type of pass and safety margin.

How it behaves when cutting

11SMnPb30 carries around 0.3% sulphur, which forms manganese sulphides, and 0.2-0.35% lead. Both act as an internal lubricant and as weak points that break the chip into small commas. The result is the best machinability of any steel: lower cutting forces, less heat at the edge and far longer tool life than in a 1018 / S235. Its weak spot is low speed: below about 150 m/min (500 SFM) material welds onto the edge (built-up edge) and the finish suffers. Here, running fast does not just produce more parts, it also leaves a better surface.

Keys to machining it in the shop

Why it machines so well: sulphur and lead

Sulphur and lead are not there for strength: they are there to cut better. Manganese sulphides stretched along the rolling direction and lead particles break the chip, lower friction on the insert face and reduce edge temperature. In exchange, the steel is less tough in the transverse direction and does not weld well. That is why it is used for lightly loaded high-volume turned parts (fittings, bushings, small shafts, special screws) and not for parts loaded in fatigue or parts that need welding.

Leaded or lead-free: 11SMnPb30 vs 11SMn30 / 1215

11SMn30 (1.0715) is the same base without lead, close to American 1215. It still machines well, but a little worse: slightly longer chips and less tool life, so plan on 10-20% less cutting speed. In Europe, lead in machining steel is allowed up to 0.35% through an environmental exemption that is reviewed periodically, and some automotive and food customers already ask for lead-free steel. Confirm it on the order before buying the bar, because switching material halfway through a run means re-tuning the program.

Swiss-type and screw machines: long runs without stopping

This steel shines on screw machines and sliding-headstock lathes: with chips that break on their own there is no need to stop and clear bird's nests, and the machine can run for hours unattended. To make the most of it, program a high, steady speed, use inserts with a chipbreaker for light finishing and watch the part-off: it is the hardest operation, because the diameter drops to zero at the end of the cut and so does the cutting speed. Constant surface speed with G96 and an rpm clamp (G50 or G92 depending on the control) keeps the spindle from running away at the centre.

Quick shop tips

  • Keep the cutting speed high: below about 150 m/min (500 SFM) built-up edge appears and the finish suffers.
  • Do not use it for welded parts or parts heavily loaded in fatigue: sulphur and lead reduce toughness.
  • If the customer wants lead-free steel, 11SMn30 / 1215 machines similarly at 10-20% less speed.
  • When parting off, clamp the rpm with G96 so the spindle does not run away at the centre.
  • Extract coolant mist at the cutting zone: good ventilation matters when machining leaded steel.

Frequently asked questions

Are 11SMnPb30, 1.0718 and 12L14 the same steel?

They are equivalent in practice: 11SMnPb30 is the EN name, 1.0718 its material number and 12L14 the closest American grade. 12L14 has slightly less carbon and sulphur, but they machine very much alike.

Can 12L14 be case hardened or hardened?

It is not designed for it. Light case hardening is possible on undemanding parts, but sulphur and lead give a poorer case. If the part needs heat treatment, a free-machining case hardening grade or 16MnCr5 / 5115 is a better choice.

Why does my 12L14 part have a poor surface finish?

Almost always because the speed is too low: at low cutting speed the material welds to the edge and tears the surface. Raise the speed above 200 m/min (650 SFM), use a sharp finishing insert and do not drop the feed below what the nose radius needs.

What cutting speed with HSS tools?

With HSS, around 60-90 m/min (200-300 SFM) for turning and 40-60 m/min with drills. Much less than with carbide, but still one of the easiest steels to cut with high-speed steel.

Can 12L14 be welded?

It is not recommended. Sulphur and lead cause cracks and porosity in the weld. If the part is welded, choose a structural steel such as 1018 / S235 or 1045 and accept that it will machine somewhat worse.

Similar materials