Skip to content
Back to Cutting parameters calculator

303 / 1.4305 stainless steel speeds and feeds

303 stainless steel (1.4305) is turned at 150-230 m/min (about 490-750 SFM) with 0.25 mm/rev using coated carbide, milled at 90-150 m/min with 0.09 mm/tooth, drilled at 105-173 m/min with 0.13 mm/rev and threaded at 53-104 m/min. It is the go-to stainless for turned parts: added sulphur breaks the chip and lets you run noticeably faster than 304, in exchange for somewhat lower corrosion resistance.

Designation
EN X8CrNiS18-9 / 1.4305 · AISI 303
Hardness
200 HB
ISO group
Stainless (M)
Turning Vc
150–230 m/min

Which operation are you machining?

Recommended speeds and feeds

Turning

150–230 m/min

0.25 mm/rev

150-230 m/min at 0.25 mm/rev for roughing with a stainless (ISO M) grade. For finishing, 0.1-0.15 mm/rev with a small nose radius and a sharp edge. Do not let the insert rub without cutting on very light passes: it work hardens less than 304, but the hardened layer is still there.

Milling

90–150 m/min

0.09 mm/tooth

90-150 m/min at 0.09 mm/tooth. Climb mill with enough chip thickness. Carbide end mills with a stainless geometry and plenty of coolant give the best tool life.

Drilling

105–173 m/min

0.13 mm/rev

105-173 m/min and 0.13 mm/rev with a through-coolant carbide drill. With cobalt HSS-E drills, around 15-25 m/min (50-80 SFM). Do not let the drill dwell in the hole: the bottom work hardens and the next pass is much harder.

Threading

53–104 m/min

0.13 mm/rev

53-104 m/min for single-point threading with carbide. With taps, 303 is far easier than 304: the short chip clears without jamming. Use a stainless tap at about 6-12 m/min with tapping oil.

Starting values for coated carbide in medium cutting. Fine-tune them in the calculator for your tool, type of pass and safety margin.

How it behaves when cutting

303 is a 304 with at least 0.15% sulphur added. That sulphur forms manganese sulphides that break up the chip and reduce friction, so the long, sticky chip typical of austenitic stainless comes out short and manageable. It is still an austenitic grade: it conducts heat poorly and work hardens if the edge rubs instead of cutting, though much less than 304. The rule is the same as for any stainless, a sharp edge and enough feed, but with more room to raise the speed.

Keys to machining it in the shop

303 vs 304: when each one pays off

303 machines much better than 304: more speed, short chips and less wear. In exchange, the sulphur lowers corrosion resistance (especially against chlorides and marine environments), makes it hard to weld and spoils polishing. It is the logical choice for high-volume turned parts going into a normal environment: shafts, bushings, fittings, screws and machine parts. If the part will be welded, exposed to salt water or mirror polished, ask for 304 or 316 and accept a longer cycle time.

Chips and coolant on Swiss-type lathes

On screw machines and sliding-headstock lathes, 303 is the stainless that lets you run without stopping to clear chips. Even so, the chip is longer than in a free-machining carbon steel: use an insert with a chipbreaker designed for stainless and enough coolant pressure to push the chip away from the cut. Stainless conducts little heat, so coolant does more than cool the edge: it also keeps the part from growing and measuring differently when finished than when it cools down.

Passivation and finishing the part

Machining leaves iron particles from the tool and open sulphides on the surface that can start to rust. That is why 303 parts going into humid environments are usually passivated after machining, a chemical treatment that cleans the surface and restores the protective layer. If the parts will be passivated, tell the processor: 303 needs a process adapted to its sulphur, because a bath designed for 304 can pit the surface.

Quick shop tips

  • For high-volume turned parts, 303 lets you run 20-30% faster than 304.
  • Do not choose 303 if the part is welded, goes to sea or is mirror polished: use 304 or 316.
  • Enough feed and a sharp edge: it work hardens less than 304, but still does not tolerate rubbing.
  • Use a stainless chipbreaker and good coolant pressure on Swiss-type lathes.
  • If parts are passivated, ask for a process suitable for sulphur-bearing stainless.

Frequently asked questions

What is the difference between 303 and 304 stainless?

The base chemistry is the same, but 303 has added sulphur. That makes it much easier to machine, at the cost of lower corrosion resistance, poorer weldability and poorer polishing. 304 is more versatile; 303 is more productive on the lathe.

Are 303, 1.4305 and X8CrNiS18-9 the same?

Yes: 303 is the AISI name, 1.4305 the European material number and X8CrNiS18-9 its EN name. Mill certificates may show any of the three.

Is 303 stainless magnetic?

Not in the annealed condition, because it is austenitic. It can become slightly magnetic in heavily cold-worked areas, such as rolled threads or cold-drawn bar, without that meaning the material is wrong.

Can 303 be welded?

It is not recommended. Sulphur causes hot cracking in the weld. If the part must be welded, use 304 or 304L.

What SFM for 303 with HSS?

With high-speed steel, around 25-40 m/min (80-130 SFM) for turning and 15-25 m/min with cobalt drills, always with plenty of coolant.

Similar materials