Skip to content
Back to Cutting parameters calculator

D2 / 1.2379 tool steel speeds and feeds

D2 tool steel (1.2379, X153CrMoV12) in the annealed condition is turned at 100-160 m/min (about 330-525 SFM) with 0.2 mm/rev using coated carbide, milled at 80-140 m/min with 0.07 mm/tooth and drilled at 70-120 m/min with 0.1 mm/rev. It is the most common steel for cold work dies, punches and shear blades: it arrives annealed at around 250 HB, is machined in that state and then hardened to 58-62 HRC.

Designation
EN X153CrMoV12 / 1.2379 · AISI D2
Hardness
250 HB (annealed)
ISO group
Steel (P)
Turning Vc
100–160 m/min

Which operation are you machining?

Recommended speeds and feeds

Turning

100–160 m/min

0.2 mm/rev

100-160 m/min at 0.2 mm/rev in the annealed condition, with a wear-resistant coated grade. Avoid very light passes that only rub: the carbides wear the edge anyway and you are not cutting. If the material is already hardened, switch to hard turning with CBN.

Milling

80–140 m/min

0.07 mm/tooth

80-140 m/min at 0.07 mm/tooth annealed. Climb mill with enough chip thickness for the edge to cut below the most abrasive layer. Hardened (58-62 HRC), mill with carbide for hard materials, a small radial step and speeds around 60-120 m/min.

Drilling

70–120 m/min

0.1 mm/rev

70-120 m/min and 0.1 mm/rev with a carbide drill. Always drill in the annealed condition: a hole in hardened D2 is an EDM job. Leave fit holes undersize so they can be ground after hardening.

Threading

35–72 m/min

0.1 mm/rev

35-72 m/min for single-point threading with carbide. For tapping, do it annealed with coated HSS-E taps at low speed (6-10 m/min). Threads in hardened parts are cut before hardening or made by EDM.

Starting values for coated carbide in medium cutting. Fine-tune them in the calculator for your tool, type of pass and safety margin.

How it behaves when cutting

D2 carries about 1.5% carbon and 12% chromium, plus molybdenum and vanadium. That combination forms a large amount of very hard chromium carbides throughout the steel, which give it great wear resistance in the die and which, when machining, act like an abrasive against the insert. Even though the annealed hardness looks moderate, the edge wears much faster than in a structural steel of the same hardness: flank wear is what governs. That is why speeds are lower than the hardness alone would suggest.

Keys to machining it in the shop

Chromium carbides: why the edge wears so fast

In D2, more than 10% of the volume is extremely hard chromium carbide, harder than many coatings. When cutting, the edge has to go through them one after another, which produces steady flank wear even though the annealed steel is only about 250 HB. In practice, use a carbide grade with a thick abrasion-resistant coating, run at the low end of the speed range for long parts and change inserts by wear, not by time.

Heat treatment: leave grinding stock

D2 is hardened in air or vacuum from about 1,020-1,080 °C and tempered, usually twice. It is a low-distortion steel, but it still moves a little and also changes volume slightly. The usual route is to rough annealed, stress relieve large parts, semi-finish leaving stock (around 0.2-0.3 mm per side on functional surfaces) and finish after hardening by grinding, hard milling or EDM.

Wire EDM of dies after hardening

D2 blanking dies are usually wire cut after hardening. To keep the part from cracking or distorting as the wire removes material, a high temper (above about 500 °C) is recommended because it reduces internal stress, and wire start holes should be drilled before hardening. If the temper was low, a large wire cut can release stress and break the die: check with your heat treater.

Quick shop tips

  • Do as much machining as possible annealed: drill and tap before hardening.
  • Check the insert for flank wear: the carbides wear it even though the steel looks soft.
  • Leave grinding stock on functional surfaces for after hardening.
  • Drill wire start holes before heat treatment.
  • If the die goes to wire EDM, ask for a high temper to reduce cracking risk.

Frequently asked questions

Are D2, 1.2379 and X153CrMoV12 the same steel?

In practice, yes: X153CrMoV12 is the EN name, 1.2379 its material number and D2 the AISI equivalent. The chemistries are very close; some mills sell branded versions with small variations.

How hard is D2 as supplied?

It is supplied annealed, at most around 255 HB. That is the hardness you machine at. After hardening and tempering it reaches 58-62 HRC depending on the temper.

Can hardened D2 be milled?

Yes, with carbide end mills for hard materials, a small radial step and a rigid machine. It is common for finishing dies, although complex shapes and holes are usually made by EDM.

What is the difference between D2 and D3 (1.2080)?

D3 / 1.2080 (X210Cr12) has more carbon and chromium but no molybdenum or vanadium. It is more wear resistant but less tough and harder to heat treat. D2 is better balanced and is the most used grade in die making.

What SFM for annealed D2 with HSS?

Around 12-20 m/min (40-65 SFM) with cobalt HSS-E drills or end mills. It is a very tough steel for high-speed steel: for production runs, carbide pays off.

Similar materials